How socket fusion joins PPR-C pipe and fittings
PPR-C pipes and fittings are joined by heat fusion: the pipe end and the fitting socket are heated on a welding machine, then pushed together so the material fuses into one piece. Connecting a pipe and a fitting by melting takes only a few seconds, and a few minutes later the welded installation is ready to be installed.
The welding temperature is 260 °C ±10 °C. When polypropylene cools down, the weld keeps its structure, shape and durability. The quality and service life of the whole installation depend equally on the geometric accuracy of the line and on the quality of every weld, so the times below matter.
This applies to all PPR-C pipes and fittings in our range, for example PN20 pipe, sockets and 90° elbows.
Welding times by pipe diameter (Ø16–75 mm)
The table gives the insert depth, heating time, processing time and cooling time for each outside pipe diameter, as published in our technical catalogue. Heating time is how long the pipe and the fitting stay on the heated tool; processing time is the time available to join them; cooling time is how long the joint is left before it is loaded.
PPR-C socket fusion times at 260 °C ±10 °C
| Outside pipe Ø (mm) | Insert depth (mm) | Heating time (s) | Processing time (s) | Cooling time (min) |
|---|---|---|---|---|
| Ø16 | 13 | 5 | 4 | 2 |
| Ø20 | 14 | 5 | 4 | 2 |
| Ø25 | 15 | 7 | 4 | 2 |
| Ø32 | 16.5 | 8 | 6 | 4 |
| Ø40 | 18 | 12 | 6 | 4 |
| Ø50 | 20 | 18 | 6 | 4 |
| Ø63 | 24 | 24 | 8 | 6 |
| Ø75 | 26 | 30 | 10 | 8 |
Step by step: welding a PPR-C joint
Follow these steps for every joint:
- Choose the heating head (die) that matches the pipe diameter and fit it on the welding machine.
- Switch on the welding machine and wait while the two control indicators are heating. When the indicator turns off, the machine has reached the welding temperature of 260 °C ±10 °C and is ready to use.
- Cut the pipe to length and attach the pipe end and the fitting properly to the welding tool. If the pipe or the fitting is dirty, clean it first with a water and alcohol solution. For aluminium-foiled pipe, the preparation method (scraping, etc.) depends on the product.
- Heat the pipe and the fitting equally, at the same time, for the heating time given in the table for that diameter.
- Remove both parts from the tool and join them within the processing time. Do not twist or move the joint after joining: this can weaken the weld.
- Leave the joint to cool for the cooling time in the table so that the weld is successful.
Common welding mistakes and how to avoid them
Most failed joints come from a few avoidable errors:
- Underheating. Too short a heating time, or a machine that has not reached temperature, gives a weak joint.
- Overheating. Too long a heating time causes internal narrowing at the weld. Pushing too hard, or using the wrong head or an incorrect technique, has the same effect.
- Moving the joint. Twisting or adjusting the parts after joining weakens the weld.
- Uncalibrated equipment. Machine and head calibration is important; check it regularly.
- Cold weather. Welding is possible, but heating and cooling times and ambient conditions become more critical. Protect the work area from wind and sudden cooling.
How to check that a weld is good
A good weld forms a smooth, even bead around the joint, with no burrs and no burning. Before the line is covered with plaster or screed, a pressure test is mandatory, and the joint must pass it without leaks. If a tested line leaks later, typical causes are a weak weld, impact damage after the test, expansion stress, a loosened threaded joint or other installation errors.
Choosing the right pipe is the other half of a reliable line: see our guide to PPR pipe pressure classes PN16, PN20 and PN25, and use the heat-fusion time calculator on site.
Request a quote
Send us the diameters, pipe classes, fittings and quantities you need through the quote request form, or contact our export team for the price list and technical documents.